02-05-2018, 11:35 PM
In any metal requiring that tight a bend, I'd be inclined to go with forging. Cherry red, hammer it over the edge of the anvil, reheat and repeat for the other bend. It may be advisable to 'upset' the bends slightly, if full strength of the 5/16" stock is required. After forging, heat it again and allow it to cool slowly to relieve stress. Then, if required, harden and temper to suit the desired characteristics.
Mike
If you can't get one, make one.
Hawkeye, proud to be a member of MetalworkingFun Forum since Jan 2013.
If you can't get one, make one.
Hawkeye, proud to be a member of MetalworkingFun Forum since Jan 2013.